Post: # 90739Post Mad_angler1

Hi guys new here but followed this site extensively, just laid 3 weeks ago 50msq of block paving in the garden. It's a rectangle walled in on a angle as the whole garden runs back towards the house, about 3ft rise from top to bottom, could not lay it level due to garage at top, at the bottom end it meets a wall that drops 4ft to the next level. On one side of the wall steps are cut into it and along the rest of the wall in iv installed drainage channel that moves water down to the next level

The problem I have is after rain we have had in the last 2 days some of the blocks in front of the steps have sunk when stepped on, iv lifted a few and the bedding layer has basically liquified.

It all was installed with between 100 and 150mm of MOT1 on top of fabric and stone dust bedding layer at a minimum of 25mm but at this particular point it's quite deep around 80mm as I had to make up to the level of the steps,

Not sure what to do next, after some checks this dust does not seem to react well with water just goes to mush, it was recommended by Travis perking as the stuff every one uses so I'm not sure what to do next

Any ideas as I'm concerned the whole thing is going to go this way

Thanks in advance

Dave_L
Site Admin
Posts: 4732
Joined: Fri Jul 28, 2006 8:47 pm
Location: Somerset
Contact:

Post: # 90741Post Dave_L

Bedding layer incorrect material and much too deep.

I fear there is only one answer and you aren't going to like it - but I'll leave it to the block paving guys.
RW Gale Ltd - Civils & Surfacing Contractors based in Somerset

See what we get up to Our Facebook page

r896neo
Posts: 521
Joined: Wed Feb 22, 2012 9:38 pm

Post: # 90742Post r896neo

80mm is far too deep as you know. Quarry dust is also widely quoted by armchair tradesmen such as counter staff in merchants as ''oh this is what everyone lays on''

I was in B&Q looking for a tiny amount of MOT type 1 to finish a small job, i only needed maybe 75KG and i couldn;t find it so i asked. He took me over to the quarry dust and said, this is what you want. He then proceeded to argue with me when i told him he was totally wrong, saying all the guys that come in here use that.

As you have found to your cost it holds water like a sponge.

I'm sorry there is no easy way to say this but as Dave mentioned you should lift it and relay. The sooner you do it the cleaner the blocks will come up.

Mad_angler1
Posts: 3
Joined: Sat Jun 15, 2013 3:32 pm
Location: Wales

Post: # 90743Post Mad_angler1

Thanks guys, seriously not happy re the dust a I specifically went to order the correct sand and was told to use the dust as it was what everyone used.

What I'm hopping I will get away with os lifting that perticular part a few feet around build up with mot1 and lay those on sand.

Lifting the whole lot is not an option right now due to other things but I do appreciate your advice.

I'm hopping as it the lowest point that's adding to the problem so if I resolve that the rest will be ok.

Bob_A
Posts: 861
Joined: Wed Feb 27, 2008 9:30 pm
Location: SE London/ NW Kent

Post: # 90744Post Bob_A

Mad_angler1 wrote:it was recommended by Travis perking as the stuff every one uses so I'm not sure what to do next
Sounds typical of my local TP who took over my very good independent builders merchant and fecked it up.

Bet you was charged way over the odds as well
:(

seanandruby
Site Admin
Posts: 4713
Joined: Mon Jun 26, 2006 11:01 am
Location: eastbourne

Post: # 90745Post seanandruby

Photos would be good. You need to lift and relay.
sean

Dave_L
Site Admin
Posts: 4732
Joined: Fri Jul 28, 2006 8:47 pm
Location: Somerset
Contact:

Post: # 90748Post Dave_L

Yes I'm sure a localised lift and relay making sure the bedding is at the correct layer thickness will remedy the problem in the short term.

Don't worry, us professionals don't always get it right..............
RW Gale Ltd - Civils & Surfacing Contractors based in Somerset

See what we get up to Our Facebook page

lutonlagerlout
Site Admin
Posts: 15184
Joined: Fri Aug 04, 2006 12:20 am
Location: bedfordshire

Post: # 90751Post lutonlagerlout

as said
lift and relay the affected areas with type 1 and 35mm of compacted grit sand
LLL
"what,you want paying today??"

YOUR TEXT GOES HERE

Mad_angler1
Posts: 3
Joined: Sat Jun 15, 2013 3:32 pm
Location: Wales

Post: # 91555Post Mad_angler1

Hi guys got another question. I used 4 pallets to do the top section of the garden. After laying I noticed we had a distinct colour diferance between the first 2 pallets and the second two, they were delivered 2 days apart from the same place, as we finished the first two almost on a straight line its very noticeable, the fist ones almost look wet compared to the second ones that look far drier

I'm hoping it will weather out but any ideas

see below pick

Image

rimexboy
Posts: 916
Joined: Thu Aug 07, 2008 8:31 pm

Post: # 91556Post rimexboy

The best you can do now is try and mix them in...

When you buy x amount you mix as you lay to avoid what you have got now..

mickg
Posts: 2598
Joined: Wed Apr 08, 2009 8:01 am
Location: Peoples Republic of Westhoughton
Contact:

Post: # 91558Post mickg

you should always lay from 2 - 3 packs of block at the same time so they are blended together, the effect what you have got is because you laid 1 pack at a time
Crystalclear
Driveway and Patio Installer

Call us today
01942 840109
7 days a week 8am till 8pm

Driveways Patios and Paving Specialists
Driveways

TheRockConcreting
Posts: 169
Joined: Wed Nov 28, 2012 4:26 pm
Location: Cambridgeshire

Post: # 91559Post TheRockConcreting

It's not something i've ever done, but won't sealing solve this problem?
Jay Johnston

The Rock Concreting Ltd
Cambridgeshire, UK

lutonlagerlout
Site Admin
Posts: 15184
Joined: Fri Aug 04, 2006 12:20 am
Location: bedfordshire

Post: # 91560Post lutonlagerlout

as mick said you should always mix from all the packs at once
however the darker ones just look a bit wetter to me
give it a while and they will blend
LLL
"what,you want paying today??"

YOUR TEXT GOES HERE

Dave_L
Site Admin
Posts: 4732
Joined: Fri Jul 28, 2006 8:47 pm
Location: Somerset
Contact:

Post: # 91582Post Dave_L

I'd give it a summer and towards the end when the blocks are as dry as can be, seal them with a sealant.

I know the pros here don't endorse it but I had a similar problem and sealed the driveway with Thomsons Driveway Seal (in a gold can) and it sorted the problem, the customer was happy.

Making sure the blocks are dry is the key here otherwise you are just sealing in moisture which will cause you grief.....