Flag loose after freeze

Patio flagstones (slabs), concrete flags, stone flags including yorkstone and imported flagstones.
dr benway
Posts: 8
Joined: Sun Jan 17, 2010 4:29 pm
Location: yorkshire

Post: # 45069Post dr benway

long time lurker, second time poster :laugh: :laugh:

after the ground being frozen solid here/under snow/ice for 3-4 weeks, sandstone flags laid in october on full mortar beds are now loose.

it doesnt appear that the beds have crumbled, just that they're now "unstuck".

whats the best way to reseat them please?

I was also thinking about repointing with rompox/romex, but please see my other post for questions about that.

any advice much appreciated

Thanks!

lutonlagerlout
Site Admin
Posts: 15184
Joined: Fri Aug 04, 2006 12:20 am
Location: bedfordshire

Post: # 45099Post lutonlagerlout

if they have "come loose" then all the bedding needs to be cut back to sub base and rebedded
sorry there is no easy fix
in all honesty the weather has been out of the ordinary ,but there has been talk of using bond bridging techniques when using sandstone
LLL
"what,you want paying today??"

YOUR TEXT GOES HERE

DNgroundworks
Posts: 1951
Joined: Sat Dec 06, 2008 10:28 pm
Location: Preston, Lancashire

Post: # 45102Post DNgroundworks

I do like using a bondbridge, a cement slurry with a SBR mixed in is what i used on sandstone painted directly on the back of the flag.....just to be sure ;)

dr benway
Posts: 8
Joined: Sun Jan 17, 2010 4:29 pm
Location: yorkshire

Post: # 45115Post dr benway

thanks all, for the replies

Is their a preferred brand of SBR?

the flags were painted with PVA, and PVA was added to the mortar-- obviously to no avail -- but as you say, it has been very, very cold.


thanks

lutonlagerlout
Site Admin
Posts: 15184
Joined: Fri Aug 04, 2006 12:20 am
Location: bedfordshire

Post: # 45123Post lutonlagerlout

I have had good results with PVA in the past ,although apparently its not recommended
can you post a picture of the bedding under the flags?
if there was any void at all and water got there,it would freeze and expand ===> popping the flags up
LLL
"what,you want paying today??"

YOUR TEXT GOES HERE

Craig2
Posts: 31
Joined: Thu Jul 24, 2003 10:39 pm
Contact:

Post: # 45161Post Craig2

I went back to work today for the first time since 4th Dec to find the frost has blown 60% of my 4" double cobble borders(about 300) gutted! the Flags seem ok and 40% of the cobbles are holding on.I laid them in November with PVA and Frostproofer in the mix and dipped the cobbles in 50/50 PVA before laying but it would seem the severity of the frost has caused the problem.
I laid the Flags pretty much the same, full bed and painted with a 50/50 PVA before being laid and touch wood they are ok.
I was looking at using something like this to refix them
http://www.rockbond.co.uk/datashe....r07.pdf

any thoughts?

I have real trouble if i have to take out all the mortar and relay the cobbles as the mortar is tight in with the Flags and I can't see it being done without causing further damage.

GB_Groundworks
Site Admin
Posts: 4420
Joined: Sat Aug 09, 2008 3:55 pm
Location: high peak
Contact:

Post: # 45180Post GB_Groundworks

run a cut off saw along the flag edge cutting the mortar to stop any cracks spreading as you pull it up but i'd be tempted to relay them all now so your not having future problems lay them with sbr in the mix and on a stronger mix(more cement), did you use sharp sand or builders sand?
Giles

Groundworks and Equestrian specialists, prestige new builds and sports pitches. High Peak, Cheshire, South Yorkshire area.

http://www.gbgroundworks.com

cookiewales
Posts: 1270
Joined: Mon Aug 10, 2009 8:30 am
Location: york work anywhere where the stone takes me
Contact:

Post: # 45188Post cookiewales

lads you should not use pva on any paving or in mortar for pointing at all its a big no no as it emullsifies on contact with water and then looks like you have poured milk over your job as for the best in my exp ronofix but all sbr should be to a standerd unibond is good but to pricey :p :;):
Originalstonepaving.com

The very best in natural stone paving in new and reclaimed materials
M: 07968 582231

Tony McC
Site Admin
Posts: 8346
Joined: Mon Jul 05, 2004 7:27 pm
Location: Warrington, People's Republic of South Lancashire
Contact:

Post: # 45201Post Tony McC

Returning to the question asked by the OP, I'd leave the flags well alone until I was sure there was actually a problem. They may have de-bonded from the bed, but unless they are actively rocking and/or moving, lifting and re-laying could well be unnecessary additional work.
Site Agent - Pavingexpert

lutonlagerlout
Site Admin
Posts: 15184
Joined: Fri Aug 04, 2006 12:20 am
Location: bedfordshire

Post: # 45225Post lutonlagerlout

i thought unibond was PVA?
definitely wouldn't use any additives in the pointing,even the dyes leach out fast
LLL
"what,you want paying today??"

YOUR TEXT GOES HERE

Craig2
Posts: 31
Joined: Thu Jul 24, 2003 10:39 pm
Contact:

Post: # 45268Post Craig2

I use Plastering sand which gives me an extra body to my mix, never had a problem with my Flagging.

I trialed a few cobbles today with an SBR Slurry bonding mix. 50/50 with OPC, I will report back my findings.

eyup Tony, its been a while :p you still on the Boddingtons?

GB_Groundworks
Site Admin
Posts: 4420
Joined: Sat Aug 09, 2008 3:55 pm
Location: high peak
Contact:

Post: # 45272Post GB_Groundworks

plastering sand is this a southern name for sharp sand?

i always use sharp sand bigger grains give better interlock stronger mix.

or plastering sand as in what you use to make a sand cement render?
Giles

Groundworks and Equestrian specialists, prestige new builds and sports pitches. High Peak, Cheshire, South Yorkshire area.

http://www.gbgroundworks.com

Craig2
Posts: 31
Joined: Thu Jul 24, 2003 10:39 pm
Contact:

Post: # 45275Post Craig2

Southern?? how very rude! :p I am more northern than most. :D
Plastering sand is a mix of both building and fine sharp (not as rough as cardewmires?)giving the best of both worlds, the stickability of building sand with added strength from the sharp.

msh paving
Site Admin
Posts: 1854
Joined: Tue Aug 19, 2008 7:03 pm
Location: kings lynn norfolk
Contact:

Post: # 45278Post msh paving

in norfolk alot off people call it medium sharp, as it is not to sharp but not soft MSH :)
paving, mini-crusher, mini-digger hire and groundwork
http://mshpaving.co.uk

cookiewales
Posts: 1270
Joined: Mon Aug 10, 2009 8:30 am
Location: york work anywhere where the stone takes me
Contact:

Post: # 45280Post cookiewales

lutonlagerlout wrote:i thought unibond was PVA?
definitely wouldn't use any additives in the pointing,even the dyes leach out fast
LLL
unibond is a sbr in most cases take a look on the tin :p ??? ???
Originalstonepaving.com

The very best in natural stone paving in new and reclaimed materials
M: 07968 582231